S136 Steel: Properties and Key Applications in Molding

Table Of Content

Table Of Content

S136 steel, also known as stainless mold steel, is a high-performance tool steel primarily used in the manufacturing of molds and dies. Classified as an austenitic stainless steel, S136 is characterized by its high corrosion resistance, excellent polishability, and good machinability. The primary alloying elements in S136 include chromium (Cr), nickel (Ni), and molybdenum (Mo), which contribute significantly to its properties.

Comprehensive Overview

S136 steel is designed for applications requiring high wear resistance and corrosion protection. Its composition typically includes around 13% chromium, 0.3% carbon, and 1% molybdenum, which enhance its hardness and toughness. The steel is often used in the production of molds for plastic injection, where the ability to withstand high temperatures and corrosive environments is critical.

Advantages:
- Corrosion Resistance: S136 exhibits excellent resistance to rust and corrosion, making it suitable for use in humid or chemically aggressive environments.
- High Hardness: The steel can achieve high hardness levels, which is beneficial for wear resistance in mold applications.
- Polishability: S136 can be polished to a high finish, which is essential for aesthetic applications and reducing friction in mold surfaces.

Limitations:
- Cost: S136 is generally more expensive than other tool steels due to its alloying elements and processing requirements.
- Weldability: While it can be welded, special precautions must be taken to avoid cracking and ensure proper joint integrity.

Historically, S136 has gained popularity in the mold-making industry due to its superior performance compared to traditional carbon steels. Its unique properties have positioned it as a preferred choice for high-quality molds, particularly in the plastic industry.

Alternative Names, Standards, and Equivalents

Standard Organization Designation/Grade Country/Region of Origin Notes/Remarks
UNS S13600 USA Closest equivalent to AISI 420
AISI/SAE AISI 420 USA Minor compositional differences
ASTM ASTM A681 USA Specification for stainless tool steels
EN EN 1.2083 Europe Equivalent grade with similar properties
JIS JIS SUS420J2 Japan Similar corrosion resistance but different mechanical properties

The table above highlights various standards and equivalents for S136 steel. Notably, while AISI 420 is often considered an equivalent, it may not provide the same level of corrosion resistance or polishability, which are critical in mold applications.

Key Properties

Chemical Composition

Element (Symbol and Name) Percentage Range (%)
C (Carbon) 0.30 - 0.40
Cr (Chromium) 12.0 - 14.0
Ni (Nickel) 0.5 - 1.0
Mo (Molybdenum) 0.5 - 1.0
Mn (Manganese) 1.0 max
Si (Silicon) 1.0 max
P (Phosphorus) 0.03 max
S (Sulfur) 0.03 max

The primary alloying elements in S136 steel play crucial roles:
- Chromium: Enhances corrosion resistance and hardness.
- Nickel: Improves toughness and ductility.
- Molybdenum: Increases hardness and resistance to pitting corrosion.

Mechanical Properties

Property Condition/Temper Test Temperature Typical Value/Range (Metric) Typical Value/Range (Imperial) Reference Standard for Test Method
Tensile Strength Annealed Room Temp 600 - 800 MPa 87 - 116 ksi ASTM E8
Yield Strength (0.2% offset) Annealed Room Temp 400 - 600 MPa 58 - 87 ksi ASTM E8
Elongation Annealed Room Temp 10 - 15% 10 - 15% ASTM E8
Hardness (HRC) Annealed Room Temp 30 - 40 HRC 30 - 40 HRC ASTM E18
Impact Strength Annealed -20°C 30 - 50 J 22 - 37 ft-lbf ASTM E23

The mechanical properties of S136 steel make it suitable for applications involving significant mechanical loading. Its high tensile strength and yield strength ensure structural integrity under stress, while its elongation indicates good ductility, allowing for deformation without fracture.

Physical Properties

Property Condition/Temperature Value (Metric) Value (Imperial)
Density Room Temp 7.8 g/cm³ 0.282 lb/in³
Melting Point/Range - 1400 - 1450 °C 2552 - 2642 °F
Thermal Conductivity Room Temp 25 W/m·K 14.5 BTU·in/(hr·ft²·°F)
Specific Heat Capacity Room Temp 500 J/kg·K 0.12 BTU/lb·°F
Electrical Resistivity Room Temp 0.72 µΩ·m 0.0000013 Ω·in

Key physical properties such as density and melting point are significant for processing and application. The relatively high melting point allows S136 to maintain its integrity at elevated temperatures, making it suitable for high-temperature applications.

Corrosion Resistance

Corrosive Agent Concentration (%) Temperature (°C/°F) Resistance Rating Notes
Chlorides 3-10 20-60 / 68-140 Good Risk of pitting
Acids 10-20 20-40 / 68-104 Fair Susceptible to stress corrosion cracking
Alkaline Solutions 5-15 20-60 / 68-140 Excellent Resistant to alkaline environments
Atmospheric - - Excellent Good for outdoor applications

S136 steel demonstrates excellent resistance to various corrosive environments, particularly in alkaline solutions. However, it is susceptible to pitting corrosion in chloride-rich environments and stress corrosion cracking in acidic conditions. Compared to other grades like AISI 420 and AISI 440C, S136 offers superior corrosion resistance, particularly in humid and chemically aggressive settings.

Heat Resistance

Property/Limit Temperature (°C) Temperature (°F) Remarks
Max Continuous Service Temp 300 572 Suitable for prolonged exposure
Max Intermittent Service Temp 400 752 Short-term exposure only
Scaling Temperature 600 1112 Risk of oxidation beyond this temp
Creep Strength Considerations 400 752 Begins to degrade at this temp

S136 steel maintains its mechanical properties at elevated temperatures, making it suitable for applications involving heat. However, care must be taken to avoid prolonged exposure to temperatures above 300 °C, as this can lead to oxidation and degradation of the material.

Fabrication Properties

Weldability

Welding Process Recommended Filler Metal (AWS Classification) Typical Shielding Gas/Flux Notes
TIG ER 308L Argon Preheat recommended
MIG ER 308L Argon + CO2 mix Post-weld heat treatment advised

S136 steel can be welded using standard processes like TIG and MIG. However, preheating is recommended to minimize the risk of cracking. Post-weld heat treatment can help relieve stresses and improve the overall integrity of the weld.

Machinability

Machining Parameter S136 Steel AISI 1212 Notes/Tips
Relative Machinability Index 70 100 Moderate machinability
Typical Cutting Speed 30 m/min 50 m/min Adjust for tool wear

S136 steel has moderate machinability compared to benchmark steels like AISI 1212. Optimal cutting speeds and tooling should be employed to achieve the best results, and care must be taken to avoid excessive heat generation during machining.

Formability

S136 steel exhibits good formability, allowing for both cold and hot forming processes. However, due to its high hardness, care should be taken to avoid work hardening during cold forming. Recommended bend radii should be adhered to in order to prevent cracking.

Heat Treatment

Treatment Process Temperature Range (°C/°F) Typical Soaking Time Cooling Method Primary Purpose / Expected Result
Annealing 800 - 850 / 1472 - 1562 1 - 2 hours Air Softening, improving machinability
Hardening 1000 - 1100 / 1832 - 2012 30 minutes Oil Increasing hardness
Tempering 200 - 300 / 392 - 572 1 hour Air Reducing brittleness

Heat treatment processes significantly affect the microstructure and properties of S136 steel. Annealing softens the material, enhancing machinability, while hardening increases hardness and wear resistance. Tempering is crucial to reduce brittleness and improve toughness.

Typical Applications and End Uses

Industry/Sector Specific Application Example Key Steel Properties Utilized in this Application Reason for Selection
Automotive Injection molds for bumpers High hardness, corrosion resistance Durability and longevity
Consumer Goods Molds for household items Excellent polishability, wear resistance Aesthetic finish and performance
Medical Devices Surgical instrument molds Corrosion resistance, biocompatibility Safety and hygiene

Other applications include:
- Molds for electronic components
- Food processing equipment
- Aerospace components

S136 steel is chosen for these applications due to its unique combination of hardness, corrosion resistance, and ability to achieve a high-quality finish, making it ideal for both functional and aesthetic requirements.

Important Considerations, Selection Criteria, and Further Insights

Feature/Property S136 Steel AISI 420 AISI 440C Brief Pro/Con or Trade-off Note
Key Mechanical Property High hardness Moderate hardness High hardness S136 offers better corrosion resistance than AISI 420
Key Corrosion Aspect Excellent Good Fair S136 is superior in corrosive environments
Weldability Moderate Good Poor S136 requires careful welding practices
Machinability Moderate Good Poor AISI 420 is easier to machine
Formability Good Fair Poor S136 can be formed with care
Approx. Relative Cost High Moderate Moderate S136 is more expensive due to alloying elements
Typical Availability Moderate High High S136 may not be as readily available as AISI 420

When selecting S136 steel, considerations include cost-effectiveness, availability, and specific application requirements. Its unique properties make it suitable for high-performance applications, but the higher cost and moderate machinability may limit its use in some scenarios. Understanding the trade-offs between S136 and alternative grades is crucial for optimal material selection in engineering applications.


Data Sources & Verification

Chemical composition and mechanical property values on this page are compiled from published material standards and cross-referenced against the equivalent designations listed above (UNS S13600, ASTM ASTM A681, EN EN 1.2083, JIS JIS SUS420J2). Values are typical or nominal and vary with product form, thickness, and heat treatment; confirm against the governing standard and mill test certificate before design or procurement use.

Design tools: Estimate material weight and quantities with our free bar, plate, and tube weight calculators (all steel calculators).

Technically reviewed by Dr. Zhang Zhiwei — former Senior Technical Specialist, Baosteel Group; member, Chinese Society for Metals. How we compile our data · spotted an error? Tell us and we will review it.