45# vs 55# – Composition, Heat Treatment, Properties, and Applications
Share
Table Of Content
Table Of Content
Introduction
Engineers, procurement managers, and manufacturing planners frequently must choose between medium‑carbon steels where a balance of strength, toughness, cost, and manufacturability is required. Two commonly considered grades in that domain are the Chinese designations 45# and 55# (roughly corresponding to steels with nominal carbon contents of about 0.45% and 0.55% respectively). Typical decision contexts include shaft and axle design, forgings and stamped parts, heat‑treated components, and situations where weldability must be balanced against strength and wear resistance.
The principal practical distinction between these two grades is that the higher carbon content in 55# generally produces greater achievable strength and hardenability at the expense of ductility and weldability. That tradeoff is why designers compare these grades when specifying components that require higher through‑hardening or surface hardness versus components that prioritize toughness, forming, and ease of joining.
1. Standards and Designations
- GB/T (China): 45# and 55# are common plain carbon steel grades in GB/T 699 and related standards for carbon structural steels and medium‑carbon steels.
- AISI/SAE equivalents (approximate): 45# ≈ AISI/SAE 1045; 55# ≈ AISI/SAE 1055 (nominally).
- EN (European): These grades fall into the non‑alloy carbon steel family (e.g., C45 family in EN 10083) rather than alloy, tool, stainless, or HSLA classes.
- Classification: Both are plain carbon steels (not stainless, not HSLA, not tool steel). They are typically treated as medium‑carbon steels suitable for quenching and tempering or surface hardening.
2. Chemical Composition and Alloying Strategy
| Element | Typical 45# (wt%) | Typical 55# (wt%) |
|---|---|---|
| C | 0.42 – 0.50 | 0.52 – 0.60 |
| Mn | 0.50 – 0.80 | 0.50 – 0.90 |
| Si | ≤ 0.40 | ≤ 0.40 |
| P | ≤ 0.035 | ≤ 0.035 |
| S | ≤ 0.035 | ≤ 0.035 |
| Cr | ≤ 0.25 (trace) | ≤ 0.30 (trace) |
| Ni | ≤ 0.30 (trace) | ≤ 0.30 (trace) |
| Mo | ≤ 0.08 (trace) | ≤ 0.08 (trace) |
| V, Nb, Ti, B, N | typically only trace/ppm levels unless microalloyed | typically only trace/ppm levels unless microalloyed |
Notes: - The composition ranges above are representative for common commercial 45# and 55# grades; exact limits depend on the specific national standard and producer. - Both grades are primarily carbon‑strengthened. Minor amounts of Mn and Si are present for deoxidation and strengthening; other elements are typically at trace levels unless the steel is intentionally microalloyed. - Alloying strategy: increasing carbon raises strength, hardness, and hardenability (ability to form martensite through thicker sections). Manganese contributes to tensile strength and hardenability and helps deoxidation; silicon primarily aids strength and springback but in small amounts.
3. Microstructure and Heat Treatment Response
- As‑rolled or annealed condition:
- Both grades typically show a ferrite + pearlite microstructure. 55# will have a greater volume fraction of pearlite due to higher carbon, producing higher as‑delivered hardness and strength but lower ductility.
- Normalizing:
- Normalizing refines grain size and produces a more uniform pearlitic/ferritic structure; both grades respond well, with 55# retaining higher strength.
- Quenching and tempering (Q&T):
- Quenching to form martensite and subsequent tempering is the standard route to achieve high strength–toughness combinations in both grades.
- 55# attains higher as‑quenched hardness and deeper hardening for a given quench severity because of higher carbon (and often slightly higher Mn), but it is more prone to quench‑induced cracking and requires careful tempering to recover toughness.
- Thermo‑mechanical processing:
- Forging and controlled rolling can refine microstructure and improve toughness for both grades; microalloying (V, Nb, Ti) would change response significantly if present.
- Hardenability:
- Hardenability is a function of carbon and alloying; with higher carbon and Mn, 55# generally has greater hardenability than 45#, enabling harder microstructures at larger cross‑sections.
4. Mechanical Properties
Table shows typical mechanical property ranges. Values depend strongly on nominal composition, section size, and heat treatment.
| Property (typical ranges) | 45# (normalized / typical Q&T) | 55# (normalized / typical Q&T) |
|---|---|---|
| Tensile strength (MPa) | Normalized: 550 – 700; Q&T: 700 – 1000+ | Normalized: 650 – 820; Q&T: 800 – 1100+ |
| Yield strength (0.2% offset, MPa) | Normalized: 320 – 430; Q&T: 500 – 900 | Normalized: 420 – 620; Q&T: 600 – 1000 |
| Elongation (A%) | Normalized: 12 – 18%; Q&T: 8 – 16% | Normalized: 8 – 14%; Q&T: 6 – 12% |
| Impact toughness (Charpy V, room temp, J) | Variable: 25 – 60 J (section dependent) | Variable: 15 – 45 J (section dependent) |
| Hardness (HB) | Normalized: ~160 – 210 HB; Q&T: ~200 – 320 HB | Normalized: ~190 – 240 HB; Q&T: ~240 – 350 HB |
Interpretation: - Strength: 55# can attain higher ultimate and yield strengths in equivalent conditions because of higher carbon (and greater pearlite/martensite fractions). - Toughness & ductility: 45# is generally more ductile and tougher in the as‑normalized state and is less likely to suffer embrittlement after quenching and tempering—especially for larger sections or improper tempering. - Hardness: 55# will generally produce higher hardness values both in as‑delivered and heat‑treated conditions. - All values are dependent on heat treatment (quench severity, tempering temperature/time), cross‑section, and specific chemistry.
5. Weldability
- Carbon content and hardenability are the primary weldability drivers in plain carbon steels. Higher carbon and higher hardenability increase the risk of forming hard, brittle martensite in the heat‑affected zone (HAZ), causing cold cracking unless preheat/post‑heat and appropriate filler materials are used.
- Common predictive indices:
- International Institute of Welding carbon equivalent: $$CE_{IIW} = C + \frac{Mn}{6} + \frac{Cr+Mo+V}{5} + \frac{Ni+Cu}{15}$$
- Dearden–O’Neill (Pcm) for consumable selection: $$P_{cm} = C + \frac{Si}{30} + \frac{Mn+Cu}{20} + \frac{Cr+Mo+V}{10} + \frac{Ni}{40} + \frac{Nb}{50} + \frac{Ti}{30} + \frac{B}{1000}$$
- Qualitative interpretation:
- 55# will register a higher carbon equivalent than 45# primarily because of higher carbon (and potentially slightly higher Mn), so 55# is less weldable without preheat or post‑weld heat treatment (PWHT).
- For critical welded structures, select low hydrogen consumables, enforce preheat, control interpass temperature, and consider PWHT for 55# to avoid HAZ cracking.
- 45# is easier to join and in many shop applications can be welded with moderate preheat and standard consumables.
6. Corrosion and Surface Protection
- Both 45# and 55# are non‑stainless carbon steels; intrinsic corrosion resistance is low.
- Typical protection strategies:
- Hot‑dip galvanizing for outdoor/atmospheric protection.
- Organic coatings (epoxy, polyurethane) or paints for mild environments.
- Surface treatments such as phosphating or oiling for indoor, non‑critical parts.
- For wear or sliding surfaces, hardfacing or case hardening (carburizing/nitriding followed by finishing) can be applied—carburizing may be used for 45# but is less common for 55# because of already higher carbon.
- PREN (pitting resistance equivalent number) is relevant only for stainless steels: $$\text{PREN} = \text{Cr} + 3.3 \times \text{Mo} + 16 \times \text{N}$$
- PREN is not applicable to plain carbon steels such as 45# and 55#.
7. Fabrication, Machinability, and Formability
- Machinability:
- Higher carbon in 55# increases tool wear and reduces machinability relative to 45#. Where machining speed and tool life are critical, 45# is more favorable.
- Heat‑treated hardness further reduces machinability; consider interrupted cutting and appropriate tooling for hardened conditions.
- Formability and cold working:
- 45# has better cold formability, bending, and drawing characteristics due to lower hardenability and greater ductility.
- 55# is more prone to cracking during forming and requires lower forming strain or elevated temperature/forming methods.
- Grinding, drilling, and finishing:
- Both can be finished to high tolerances, but optimum cutting parameters depend on final hardness. Surface finishing costs rise with hardness (55# heat treated parts cost more to finish).
- Heat treatment constraints:
- 55# requires more careful quench control and tempering regimes to avoid distortion/cracking in forgings and large sections.
8. Typical Applications
| 45# (Typical Uses) | 55# (Typical Uses) |
|---|---|
| Shafts, axles (moderate loads), crankshafts (when forged/tempered), couplings, general mechanical parts requiring good machinability and reasonable strength | Heavier‑duty shafts, pins, some types of gear blanks, wear parts, components requiring higher through‑hardening or higher service hardness |
| Forged and machined components that will be normalized or Q&T for moderate strength and good toughness | Components intended for higher hardness after quench & temper, including some agricultural and construction parts |
| Cold‑formed parts where ductility and bending are required | Parts subject to higher contact stresses or where higher static strength/wear resistance is prioritized |
Selection rationale: - Choose 45# where manufacturing ease, weldability, and toughness are priorities and section sizes are moderate. - Choose 55# where higher strength or deeper hardening is needed, and the production process can manage the stricter heat treatment, welding, and machining requirements.
9. Cost and Availability
- Cost:
- Both grades are commodity plain carbon steels. 45# is typically slightly cheaper due to wider use and slightly lower carbon content (and therefore easier processing).
- 55# can be marginally more expensive because of higher carbon and potentially tighter quality control for heat treatment applications.
- Availability:
- 45# is extremely common in bar, plate, and forging stock. 55# is also widely available but less ubiquitous than 45# in some markets and product forms.
- Lead times for heat‑treated, surface‑treated, or large cross‑section 55# parts may be longer due to process care (preheat schedules, tempering, controlled cooling).
10. Summary and Recommendation
| Criterion | 45# | 55# |
|---|---|---|
| Weldability | Better (lower CE) | Lower (higher CE; requires preheat/PWHT) |
| Strength–Toughness balance | Good toughness with moderate strength | Higher achievable strength, lower ductility if not tempered correctly |
| Cost | Slightly lower, more available | Slightly higher, may need stricter heat treatment controls |
Choose 45# if: - The design emphasizes ductility, impact toughness, machinability, or frequent welding. - Parts are medium cross‑section and require economic production and broad availability. - You want a forgiving heat‑treatment window and easier shop‑floor handling.
Choose 55# if: - Higher as‑delivered hardness, greater achievable tensile and yield strengths, or improved through‑hardening of thicker sections is required. - The manufacturing plan includes controlled quenching and tempering, or surface hardening where baseline carbon is advantageous. - You accept additional welding and machining precautions and possibly a small premium in material and processing cost.
Concluding note: specification should consider geometry, intended heat treatment, required surface finish, weld requirements, and in‑service loads. When in doubt, request sample heat‑treated test coupons or perform a hardness/toughness trial on representative sections before committing a full production run.